Skip to content

PROTECTING YOUR WORLD

Concrete Moisture Testing:
Is the Slab Dry
Enough to Coat?

RH probes, calcium chloride kits and plastic sheets explained, the limits floors and coatings actually use, and how many tests your slab needs.
Damp slab?

Moisture readings too high? There are options.

Send us your slab size and test results. A certified ArmorThane applicator can tell you whether the floor can be coated now, needs a moisture-tolerant primer or should wait.

  • Slab area and thickness
  • On grade, below grade or suspended
  • RH or calcium chloride readings, if you have them
  • Coating or flooring planned
Rather talk now? Call (417) 831-5090
Step 1 of 3
40%
Probe depth in a slab drying from one side
20% when it dries from two sides
24 hr
Wait after drilling before reading an RH probe
ASTM F2170
3 + 1
Tests for the first 1,000 sq ft, plus one per extra 1,000
F2170 and F1869
75%
Typical in-slab RH ceiling for epoxy and resinous coatings
Or 3 lb MVER

Concrete moisture testing is the cheapest insurance a floor coating will ever have. Slabs hold water for months after the pour, and moisture moving up from the ground never fully stops. Coat over too much of it and you get blisters, white bloom, soft adhesive and peeling, usually long after the crew has packed up. A few probes and a few days of waiting tell you whether the slab is ready.

Quick answer

The standard for concrete moisture testing is ASTM F2170: drill holes to 40% of slab depth (20% if it dries from both sides), insert RH probes, wait 24 hours and read them. Use three tests for the first 1,000 sq ft plus one per additional 1,000. Most epoxy and resinous coatings want 75% RH or lower, or an ASTM F1869 calcium chloride result of 3 lb or less.

Methods

Concrete moisture testing methods compared

Four tests show up on jobsites. Only two give numbers that a coating or flooring manufacturer will accept, and they measure different things, so they do not convert into each other.

MethodStandardTest time (hr)What it tells you
In-situ relative humidity probesASTM F217024 after drillingRH deep in the slab, where moisture will settle once it is sealed. The preferred test.
Calcium chloride domeASTM F186960–72Vapor emission rate from roughly the top 1/4 to 1/2 inch, in lb per 1,000 sq ft per 24 hours.
Plastic sheetASTM D426316 minimumYes or no: does visible moisture collect under an 18 in square of taped poly?
Electronic moisture meterASTM F2659MinutesComparative surface reading. Good for finding wet areas and placing probes, not for sign-off.
The plastic sheet and meter tests are screening tools. Acceptance numbers come from F2170 or F1869, whichever the product data sheet names. Tap a column heading to sort.
Which one to trustWhen the two quantitative tests disagree, we lean on RH probes. Calcium chloride reads the skin of the slab at one moment, while a probe at 40% depth shows what the surface will see once a coating traps the moisture in. Many flooring makers now list F2170 first for that reason.
Procedure

How to run an F2170 RH test

The method is simple. The discipline is in the conditions and the waiting, and that is where most bad readings come from.

  1. Get the building to service conditions

    The slab and the air above it should sit at normal operating temperature and humidity for 48 hours before you read. Testing a cold, unheated shell gives numbers that mean little.

  2. Lay out the holes

    Three for the first 1,000 sq ft, then one more per additional 1,000. Put one near the center and spread the rest around the room, with extra attention to wet-looking areas a meter flagged.

  3. Drill to the right depth

    40% of slab thickness for a slab on grade or over a vapor retarder; 20% for a suspended slab drying top and bottom. Vacuum the dust out, set the sleeve and cap it.

  4. Wait, then read

    Give the hole 24 hours to reach equilibrium, insert the calibrated probe and record the reading once it stabilizes. Log the date, location, slab and air temperature, and ambient RH beside each number.

Probes should carry a current calibration. Meter accuracy is usually stated at about ±2 to 3% RH, so a 74% reading against a 75% limit is a judgment call, not a clean pass.

Planner

How many tests, and did you pass?

Enter the slab and the floor system. The planner gives the number of test locations and the probe depth, then checks your highest readings against the limit. Change the limits to match your product data sheet; it is the document that counts.

Plan and check

Moisture test planner and pass/fail checker

Tests = 3 for the first 1,000 sq ft + 1 per additional 1,000 (ASTM F2170 and F1869). Probe depth = 40% of thickness for one-sided drying, 20% for two-sided. Preset limits are typical values from IFTI's moisture guidance: coatings and wood 75% RH or 3 lb, resilient flooring up to 80% or 5 lb, carpet 85% or 5 lb.

—
Test locations needed
—
Probe hole depth (in)
—
RH check
—
Calcium chloride check

Slab failed? Our concrete primer guide covers moisture-tolerant primers, and white deposits on a damp slab are explained in our efflorescence guide.

Limits

How dry is dry enough?

No ASTM test method sets a pass mark. The coating or flooring maker does, in the data sheet or installation guide. These are the typical ceilings you will see, and the reason the numbers differ is how much vapor each product can tolerate before it blisters or lets go.

Strict

Epoxy and resinous coatings

About 75% RH or 3 lb MVER. A dense, non-breathing film over a wet slab builds pressure underneath and blisters.

Strict

Wood flooring

About 75% RH or under 3 lb, and the wood itself has to be within its own moisture spec.

Moderate

Resilient flooring

Vinyl, LVT and linoleum: typically 75 to 80% RH or 3 to 5 lb, depending on the adhesive.

Tolerant

Carpet and carpet tile

Around 85% RH or 5 lb. Still check the adhesive, which is usually the weak link.

When a slab will not get there in time, moisture mitigation systems built to ASTM F3010 are the usual fix. These are high-solids epoxy membranes rated for very high slab RH, some up to 100%, which then take the coating or flooring on top. They cost more than waiting, but a lot less than tearing out a failed floor. For basements and slabs on grade with water coming through, deal with the source too; see concrete waterproofing and basement floor coatings.

Field experience

Why moisture readings mislead people

Most moisture disputes we get called into are not about the slab. They are about how and when it was tested.

  • HVAC off: a building without heat or air gives readings that change the week it is turned on. Wait for service conditions.
  • Only testing the dry spots: holes along a sunny wall miss the damp core of the room. Spread them out and add tests where a meter reads high.
  • Calcium chloride on a sealed slab: F1869 needs a clean, bare surface. Grind the test spot first, or the sealer blocks the vapor and the number reads low.
  • Trusting the 28 days: 28 days is a strength milestone, not a dryness one. Thick slabs, wet curing and cold weather can keep RH high for months.
  • Testing before prep: grinding or blasting opens the surface. If you can, confirm readings after prep and right before the primer goes down.
Polyurea and damp slabsMoisture and warming concrete also cause outgassing, the pinholes and bubbles you see when a slab breathes into a fresh film. Prime first and spray while the slab temperature is steady or falling. Prep comes before all of it, whether that is shot blasting or diamond grinding, and our surface preparation guide ties the steps together.
Coat with confidence

Readings first, then the coating.

A certified ArmorThane applicator can test your slab, explain the numbers and recommend a primer and coating system that suits them.

Contractors: become an ArmorThane applicator

FAQ

Moisture testing questions

How is concrete moisture testing done?

The preferred method is ASTM F2170: drill holes to 40% of slab depth, insert RH probes, wait 24 hours and read them. The other accepted method is the ASTM F1869 calcium chloride test, which measures vapor emission at the surface over 60 to 72 hours.

What moisture level is acceptable for epoxy on concrete?

Typical limits for epoxy and resinous coatings are about 75% in-slab RH by ASTM F2170, or 3 lb per 1,000 sq ft per 24 hours by ASTM F1869. The product data sheet sets the actual limit, and some primers are rated higher.

How long does concrete take to dry before coating?

There is no reliable calendar rule. Slab thickness, mix water, curing method, vapor retarder and building conditions all change drying time, and thick slabs can take months. The 28 day mark is about strength, not dryness, so test instead of counting days.

Is the plastic sheet test good enough?

Only as a screen. ASTM D4263 tapes an 18 inch square of plastic down for at least 16 hours and checks for visible moisture. A wet result says stop; a dry result does not prove the slab meets a coating's RH or MVER limit.

Can I use a moisture meter on concrete?

Yes, for comparison. Electronic meters, covered by ASTM F2659, read near the surface and are handy for mapping wet areas and choosing where to drill. They are not an acceptance test for coatings or flooring.

What happens if you coat concrete that is too wet?

Vapor pressure builds under the film. Common results are blisters, pinholes from outgassing, white efflorescence at the edges, soft or re-emulsified adhesive and coatings that peel in sheets. Repairs mean removing the failed system and starting over.

AT
Written by the ArmorThane technical team. We have manufactured polyurea, polyurethane and polyaspartic coatings and plural component spray equipment in Springfield, Missouri since 1989. Limits here are typical; always follow the product data sheet and the test standard for the floor you are coating.

Sources

  1. ASTM International, F2170 Standard Test Method for Determining Relative Humidity in Concrete Floor Slabs Using in situ Probes. astm.org/f2170-19a.html
  2. Floor Expert, ASTM F2170 procedure summary. floorexpert.com/knowledge-base/astm-f-2170
  3. IFTI, ASTM F1869 Calcium Chloride Moisture Test Explained. ifti.com/astm-f1869-calcium-chloride-moisture-test-explained
  4. IFTI, Concrete Moisture Testing Requirements by Flooring Type. ifti.com/concrete-floor-moisture-testing-requirements-for-different-flooring-types
  5. Wagner Meters, ASTM F2170 guideline for RH sensors per 1,000 sq ft. wagnermeters.com/concrete-moisture-test/concrete-info/astm-guideline-rh-sensor

Test first, then coat.

Certified ArmorThane applicators check the slab before they spray, so moisture does not lift the floor six months later. Contractors can add floor coatings with our equipment and training, with no franchise fee and no royalties.

United States 417-831-5090 · Canada 780-444-6200

CONTACT US

REQUEST A QUOTE OR

BECOME AN APPLICATOR

ArmorThane has built a strong reputation over the past 30 years for producing high-quality, durable protective coatings.

group 115 660555abebfe4
Phone Number

Tel: 417.831.5090

group 115 1 660556c21395c
Email Us

moreinfo@armorthane.com

Step 1 of 3

We want to help you find the best ArmorThane applicator for your protective coating project. Please either fill out the request form below or call us toll free at 417-831-5090, any time Monday-Friday, 8:00 a.m. to 5:00 p.m. Central Standard Time.

RV Find An Applicator

Protective Coating Applications

Products

Applicator Opportunities

Knowledge Center

Galleries